Stanyl® TS350
- Chemical Family
- Polyamides
Stanyl® TS350 is a high-performance polyamide that provides unmatched performance and value for demanding applications in which superior heat resistance, design stiffness, wear and friction, and process flow qualities are required. This high-performance polyamide 46 is used for applications in automotive, E&E, gears, and outdoor power equipment. Since it retains its mechanical properties at high temperatures up to 220 °C, this makes it ideal for extremely high-performance applications, where it outperforms PPA, PA6T, PA9T, and often PPS and LCP. A suitable processing technology for the product is injection molding. Special features include heat stabilization.
Product families
Applications
- Connectors
Product Families
- Polyamides
Other characteristics
- Brand
- Stanyl
- Polymer Name
- Polyamide 46 (PA 46)
- Flexural Modulus
- 3200.0 - 3200.0 MPa
- Additives Included
- Heat Stabilizer
- Processing Methods
- Injection Molding
- Safety
For the safety properties of the material, we refer to our SDS which can be ordered at our sales offices. During practical operation we advise to wear personal safety protections for hand/eye/body.
- Markets
- Electrical & Electronics
- Flame Rating
- UL 94 V0
- Technology
- Plastics
- Packaging Type
- Bags
- Boxes
- Silos
- Super Sacks
- Quality Standards
- UL Yellow Card (E172082)
- UL Yellow Card (E47960)
- Material Features
- Flame Retardant
- Heat Resistance
- Heat Stabilized
- UL Flame Rated
- Certifications and Compliance
- ISO 14001
- OHSAS
- REACH (Europe)
- UL 94
- Plastics and Elastomers Functions
- Resin
Technical data
Table 1 of 7
8 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Tensile Modulus | 3400 / - | MPa | ISO 527-1/-2 |
| Yield Stress | 80 / - | MPa | ISO 527-1/-2 |
| Yield Strain | 5 / - | % | ISO 527-1/-2 |
| Nominal Strain at Break | 7 / - | % | ISO 527-1/-2 |
| Flexural Modulus | 3200 / - | MPa | ISO 178 |
| Flexural Strength | 130 / - | MPa | ISO 178 |
| Charpy Notched Impact Strength (at +23°C) | 4 / - | kJ/m² | ISO 179/1eA |
| Charpy Notched Impact Strength (at -30°C) | 3 / - | kJ/m² | ISO 179/1eA |
Table 2 of 7
8 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Melting Temperature (10°C/min) | 295 / * | °C | ISO 11357-1/-3 |
| Glass Transition Temperature (at 10°C/min) | 75 / * | °C | ISO 11357-1/-2 |
| Temperature of Deflection Under Load (1.80 MPa) | 190 / * | °C | ISO 75-1/-2 |
| Coefficient of Linear Thermal Expansion (parallel) | 0.8 / * | E-4/°C | ISO 11359-1/-2 |
| Coefficient of Linear Thermal Expansion (normal) | 0.9 / * | E-4/°C | ISO 11359-1/-2 |
| Burning Behaviour (at 1.5 mm Nominal Thickness) | UL V-0 / * | class | IEC 60695-11-10 |
| Burning Behaviour (at 3.0 mm Nominal Thickness) | UL V-0 / * | class | IEC 60695-11-10 |
| Oxygen Index | 29 / * | % | ISO 4589-1/-2 |
Table 3 of 7
8 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Relative Permittivity (100Hz) | 3.8 / 10 | — | IEC 62631-2-1 |
| Relative Permittivity (1 MHz) | 3.5 / 4.1 | — | IEC 62631-2-1 |
| Dissipation Factor (100 Hz) | 50 / 2800 | E-4 | IEC 62631-2-1 |
| Dissipation Factor (1 MHz) | 200 / 800 | E-4 | IEC 62631-2-1 |
| Volume Resistivity | 1E13 / 1E7 | Ohm*m | IEC 62631-3-1 |
| Surface Resistivity | - / 1E14 | Ohm | IEC 62631-3-2 |
| Electric Strength | 30 / 25 | kV/mm | IEC 60243-1 |
| Comparative Tracking Index | 225 / - | V | IEC 60112 |
Table 4 of 7
2 rows| Characteristic | Value | Unit |
|---|---|---|
| Density of Melt | 1140 / * | kg/m³ |
| Thermal Conductivity of Melt | 0.24 / * | W/(m K) |
Table 5 of 7
4 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Water Absorption | 8.6 / * | % | Sim. to ISO 62 |
| Water Absorption in Water (at 23°C after 24h) | 2.4 / * | % | ISO 62 |
| Humidity Absorption | 2.35 / * | % | Sim. to ISO 62 |
| Density | 1430 / - | kg/m³ | ISO 1183 |
Table 6 of 7
2 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Molding Shrinkage (parallel) | 1.5 / * | % | Sim. to ISO 294-4 |
| Molding Shrinkage (normal) | 1.5 / * | % | Sim. to ISO 294-4 |
Химическая стойкость
377 rows| Characteristic | Value | Unit |
|---|---|---|
| Other | Acetaldehyde (40% by mass) at 23°C | resistant |
| Other | Acetamide (50% by mass) at 23°C | limited resistant, tests necessary to verify |
| Other | Acetamide (50% by mass) at >140°C | not resistant |
| Other | Acetic acid (10% by mass) at 100°C | not resistant |
| Other | Acetic acid (10% by mass) at 23°C | limited resistant, tests necessary to verify |
| Other | Acetic acid (95% by mass) at 23°C | not resistant |
| Ketones | Acetone at 23°C | resistant |
| Other | Acetophenone at 23°C | resistant |
| Other | Acetyl chloride at 23°C | not resistant |
| Other | Acetylene at 23°C | resistant |
| Other | Acrylic acid at 23°C | not resistant |
| Other | Aliphatic amines at 23°C | resistant |