To catalogue
Akulon® S223-G6
- Chemical Family
- Polyamides
Akulon® S223-G6 is a high-performance material that combines the properties of polyamide 6 and polyamide 66. It is widely utilized by customers worldwide in diverse applications, including automotive, electronics, electrical, furniture, and packaging. In molded parts, this material excels in providing an excellent balance between ease of design and processing, while delivering outstanding mechanical properties over a broad temperature range and under various conditions.
Product families
Applications
Automotive & Transportation — Automotive
- Exterior & Body
- Interior
Product Families
Plastics — Engineering & Specialty Polymers
- Polyamides
Composite Materials — Polymers & Resins
- Thermoplastic Resins
Other characteristics
- Brand
- Akulon®
- Polymer Name
- Polyamide 66 (PA 66), Polyamide Copolymer
- Polyamide 66 (PA 66)
- Polyamide Copolymer
- Fillers Included
- Glass Fiber
- Processing Methods
- Injection Molding, Injection Molding
- Reinforcement Material
- Glass Fibers
- Markets
- Automotive & Transportation
- Flame Rating
- UL 94 HB
- Technology
- Composite Materials
- Plastics
- OEM Standards
- Mercedes
- Packaging Type
- Bags
- Boxes
- Silos
- Super Sacks
- Quality Standards
- UL Yellow Card (E43392)
- UL Yellow Card (E47960)
- Material Features
- Light Weight
- UL Flame Rated
- OEM Specifications
- MERCEDES DBL 5410
- Reinforcement Form
- Tape
- Unidirectional Fabric
- Certifications and Compliance
- ISO 14001
- OHSAS
- REACH (Europe)
- UL 94
- Composite Materials Functions
- Resins Binders & Matrix Materials
- Composites Processing Methods
- Injection Molding
- Plastics and Elastomers End Uses
- Door Panel
- Flooring
- Wheel Housing Parts
- Plastics and Elastomers Functions
- Resin
- Plastics and Elastomers Processing Methods
- Injection Molding
Technical data
Table 1 of 7
16 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Tensile Modulus | 10000 / 7500 | MPa | ISO 527-1/-2 |
| Tensile Modulus (-40°C) | 10500 / - | MPa | ISO 527-1/-2 |
| Tensile Modulus (100°C) | 4850 / - | MPa | ISO 527-1/-2 |
| Stress at Break | 205 / 140 | MPa | ISO 527-1/-2 |
| Stress at Break (-40°C) | 255 / - | MPa | ISO 527-1/-2 |
| Stress at Break (100°C) | 110 / - | MPa | ISO 527-1/-2 |
| Strain at Break | 3.6 / 5 | % | ISO 527-1/-2 |
| Strain at Break (at -40°C) | 3.4 / - | % | ISO 527-1/-2 |
| Flexural Modulus | 9300 / 6400 | MPa | ISO 178 |
| Flexural Strength | 295 / 200 | MPa | ISO 178 |
| Charpy Impact Strength (at +23°C) | 80 / 100 | kJ/m² | ISO 179/1eU |
| Charpy Impact Strength (at -30°C) | 70 / 70 | kJ/m² | ISO 179/1eU |
Table 2 of 7
13 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Melting Temperature (10°C/min) | 260 / * | °C | ISO 11357-1/-3 |
| Temperature of Deflection Under Load (1.80 MPa) | 245 / * | °C | ISO 75-1/-2 |
| Temperature of Deflection Under Load (0.45 MPa) | 260 / * | °C | ISO 75-1/-2 |
| Coefficient of Linear Thermal Expansion (parallel) | 0.2 / * | E-4/°C | ISO 11359-1/-2 |
| Coefficient of Linear Thermal Expansion (normal) | 0.7 / * | E-4/°C | ISO 11359-1/-2 |
| Burning Behaviour (at 1.5 mm Nominal Thickness) | UL HB / * | class | IEC 60695-11-10 |
| Burning Behaviour (at 3.0 mm Nominal Thickness) | UL HB / * | class | IEC 60695-11-10 |
| Relative Temperature Index (Electrical, 0.71 / * mm) | 65 / * | °C | UL746B |
| Relative Temperature Index (Electrical, 3 / * mm) | 65 / * | °C | UL746B |
| Relative Temperature Index (with impact, 0.71 / * mm) | 65 / * | °C | UL746B |
| Relative Temperature Index (with impact, 3 / * mm) | 65 / * | °C | UL746B |
| Relative Temperature Index (without impact, 0.71 / * mm) | 65 / * | °C | UL746B |
Table 3 of 7
8 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Relative Permittivity (100Hz) | 3.8 / 11 | — | IEC 62631-2-1 |
| Relative Permittivity (1 MHz) | 3.5 / 4.6 | — | IEC 62631-2-1 |
| Dissipation Factor (100 Hz) | 90 / 1400 | E-4 | IEC 62631-2-1 |
| Dissipation Factor (1 MHz) | 160 / 1000 | E-4 | IEC 62631-2-1 |
| Volume Resistivity | 1E13 / 1E11 | Ohm*m | IEC 62631-3-1 |
| Surface Resistivity | - / 1E14 | Ohm | IEC 62631-3-2 |
| Electric Strength | 30 / 25 | kV/mm | IEC 60243-1 |
| Comparative Tracking Index | 600 / 600 | V | IEC 60112 |
Table 4 of 7
2 rows| Characteristic | Value | Unit |
|---|---|---|
| Thermal Conductivity of Melt | 0.172 / * | W/(m K) |
| Specific Heat Capacity Melt | 2170 / * | J/(kg K) |
Table 5 of 7
3 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Water Absorption | 6 / * | % | Sim. to ISO 62 |
| Humidity Absorption | 1.6 / * | % | Sim. to ISO 62 |
| Density | 1360 / - | kg/m³ | ISO 1183 |
Table 6 of 7
2 rows| Characteristic | Value | Unit | Method |
|---|---|---|---|
| Molding Shrinkage (parallel) | 0.2 / * | % | Sim. to ISO 294-4 |
| Molding Shrinkage (normal) | 1.2 / * | % | Sim. to ISO 294-4 |
Химическая стойкость
384 rows| Characteristic | Value | Unit |
|---|---|---|
| Other | Acetaldehyde (40% by mass) at 23°C | limited resistant, tests necessary to verify |
| Other | Acetamide (50% by mass) at 23°C | limited resistant, tests necessary to verify |
| Other | Acetamide (50% by mass) at >140°C | not resistant |
| Other | Acetic acid (10% by mass) at 100°C | not resistant |
| Other | Acetic acid (10% by mass) at 23°C | limited resistant, tests necessary to verify |
| Other | Acetic acid (95% by mass) at 23°C | not resistant |
| Ketones | Acetone at 23°C | resistant |
| Other | Acetophenone at 23°C | resistant |
| Other | Acetyl chloride at 23°C | not resistant |
| Other | Acetylene at 23°C | resistant |
| Other | Acrylic acid at 23°C | not resistant |
| Other | Aliphatic amines at 23°C | resistant |